院报 ›› 2023, Vol. 40 ›› Issue (1): 171-175.DOI: 10.11988/ckyyb.20210825

• 水工结构与材料 • 上一篇    下一篇

纳米SiO2和碳酸钙晶须制备水泥基材料性能试验

黄伟1, 张阳阳1, 葛进进2, 方张平1   

  1. 1.淮南联合大学 建筑与艺术学院,安徽 淮南 232038;
    2.安徽理工大学 土木建筑学院,安徽 淮南 232001
  • 收稿日期:2021-08-07 修回日期:2022-01-12 出版日期:2023-01-01 发布日期:2023-02-24
  • 作者简介:黄 伟( 1980-) ,男,安徽青阳人,教授,博士(后),研究方向为混凝土结构与材料。E-mail:hwaust@163.com
  • 基金资助:
    安徽省高校自然科学研究重点项目(KJ2020A0899);安徽省高校学科拔尖人才学术资助项目(gxbjZD2022111)

Properties of Cement-based Material Mixed with Nano-SiO2 and Calcium Carbonate Whisker

HUANG Wei1, ZHANG Yang-yang1, GE Jin-jin2, FANG Zhang-ping1   

  1. 1. School of Architecture and Arts,Huainan Union University,Huainan 232038,China;
    2. Institute of Civil Engineering and Architecture,Anhui University of Science and Technology, Huainan 232001,China
  • Received:2021-08-07 Revised:2022-01-12 Online:2023-01-01 Published:2023-02-24

摘要: 采用纳米SiO2和碳酸钙晶须制备水泥基材料,利用SEM、XRD和TG-DSC等技术手段对水泥基材料的水化产物、微观结构和热稳定性等进行有效表征,并试验研究了双掺0%、1%、2%、3%、5%、10%的碳酸钙晶须和1%纳米SiO2保温水泥砂浆的力学性能和导热性能。研究结果表明:纳米-毫米两种尺度材料掺入水泥浆内部后,纳米SiO2与水泥水化产物Ca(OH)2晶体发生二次水化反应,生成C-S-H凝胶体,有效地填充水泥基体孔隙、细化水泥基内部孔径尺寸,碳酸钙晶须具备纤维和微粒双重作用,可以在水泥基中产生纤维的桥联效应,两者材料结合起来,可在水泥基内部形成密实网状絮凝结构;纳米SiO2和碳酸钙晶须掺入后可以提高砂浆的强度,3%碳酸钙晶须和1%纳米SiO2配制的保温水泥砂浆抗压和抗折强度分别为25.6 MPa和6.19 MPa,导热系数为0.456 7 W/(m·K),强度和导热性能兼顾。

关键词: 纳米SiO2, 碳酸钙晶须, 微观分析, 力学性能, 导热系数

Abstract: The hydration products,microstructure and thermal stability of cement-based materials prepared by mixing with nano-SiO2 and calcium carbonate whisker were effectively characterized by using SEM,XRD and TG-DSC.The mechanical properties and thermal conductivity of thermal-insulated cement mortar were also studied by adding 0%,1%,2%,3%,5% and 10% calcium carbonate whisker and 1% nano-SiO2.Test results revealed that by adding materials of nano-and-millimeter level scales,C-S-H gels were generated from the secondary hydration reaction between nano-SiO2 and Ca(OH)2 crystal,filling the voids in cement base and refining the pores in cement base.Moreover,calcium carbonate whisker has dual-function of fibers and particles,hence producing bridging effect in the cement based,forming a dense network flocculation structure inside the cement base.The strength of cement mortar can be improved by adding nano-SiO2 and calcium carbonate whisker.The compressive strength and flexural strength of thermal insulation cement mortar mixed with 3% calcium carbonate whisker and 1% nano-SiO2 is 25.6 MPa and 6.19 MPa,respectively,and the thermal conductivity is 0.456 7 W/(m·K).Both the strength and thermal conductivity are taken into consideration.

Key words: nano-SiO2, calcium carbonate whisker, microscopic analysis, mechanical properties, thermal conductivity